Tuesday, January 4, 2011

SULPHURIC ACID TEST :


Some fabric is heated with 20% H2 so4; cool dilute, diazotise by
addition of a little sodium nitrite, couple with alkaline Rsalt solution : 
red indicates aniline from aniline formaldehyde resins. some of 
the above uniazotised solution is steam destilled into liebermann storch reagent; 
return of coloul may indicate a urea formaldehyde resin.

Fuse a little cloth with na OH, extract with water , add to about IO
c.c. of extract, two drops of a I% suspension in water of dinrom- quinone 
chlorimide; add oI % naOH solution drop by drop to ph 9.4; blue purple 
indicates phenols, cresols , xylenols and their p-tert- alkyl derivaties.

The fabtic is steeped for one hour in a saturated aqueous solution of the resgent, 
then for fifteen minutes in 20 vol. hydrogen peroxide:
mauve- brown indicates cellulose fibres and urea formaldehude resins; 
yellow indicates thermoplastic resins.


Alittle fabric is steeped for several hours in a cold soluion of kiton blue v at
ph 3.1; blue indicates lignified celluloses, urea form aldehyde resins ,and 
polyamides; no colour indicates cellulose fibres and phenol-formaldehyde types.

 (A) Scbiff;s reagent, see test 13. (b) A small piece of cloth 
is placed in 2 c.c. of 66% v/v H2SO 4,and a few crystals of cbromotropic acid heat 
at 60-70 deg, c. for ten minutes: bright violet indicates formaldeghde. 
A blank is necessary to allow for impurities in the air. (C) scbryver's 
test; to 5 c.c of solution prepared by hydrolysing resin coated fabric with 
2% HCI at the boilfor ten minutes, add I c.c. fp freshly prepared I% 
phenylhydrazine hydrochloride stand two to three minutes, add I C.c.5% 
potassium ferricyanide and 5 c.c. conc. HCI : purple red indicates formaldehyde.  
(D)To 5 c.c. of hydrolysate (as test (C) add a little pbloroglucinol and neutralise 
with NaOH : deep red indicates formaldehyde.

IO% NITRIC ACID:

This reagent discolours cellulose acetate butyrates but one cellulose acetate.

Distillation with syrupy phosphoric acid will split off acetic, pro pionic, and 
other volatile acids from combination in resins. steam destillation is advisable,
and the method may be made quantitative by following the method on p. 280.

Fusion with sodium or with Na OH produced sodium thiocyanate 
(which gives a red colour with ferric chloride ) if thiourea resins, are 
present.

NITRATION OF PHENOLS :
Alittle resin is biled with cone. HNO3, and the reaction mixture steam distilled,
yielding 0-nitrophenol, a yellow solid dessolving in Na OH solution to an intense orange 
colour; m.p. 45 deg. C.

(N.B. potassium and ammonium pocrates are explosive when dry.)
The solution from acid hydrolysis, of certain resins may be used to produce characteristic
picrates, identifiable by their melting points after rec rysteristic Coumarone piccrate:
m.p. 102 103 deg.c. indene picrate, m.p. 98 deg. c. melamine : m.p. 312 325 deg.c. candlin 
(J.S.D.C. 1947 p. 144) gives the following method for melamine /formaldehyde finishes. add 
5 cms. resin to 250 c.c. dilute H2SO4 warm to 70 deg. c. add solid potassium permanganate 
until there is no further decolorisation,filter to remove mno2 and carbonaceous matter, 
just decolorise the filtrate, add escess na Oh to precipitate dissolved mn, boil, filter, 
make neutral with H2 SO4, add excess of saturated aqueous picric acid, when the melamine 
picrate is precipitated. ( N.B. the solubility of melamin ein water is rather low.

WATER SWELLING;

Cameron and Morton's test; steep 0.5 gm. regenerated cellulose rayon in cold water,
centrifuge for five minutes at 1000 g. and weigh immediately. untreated fibres adn
borax treated fibres show 100% absorption; one per 40 glucse residues gives 35%
imbibition.

63% SULPHURIC ACID SWELLING :



Cameron and ,orton's test consists in steeping cellulose rayon
fibres for five seconds in the reagent; air five seconds, and wash with
an excess of water. uncross bonded viscose is completely parch mintised. Cross
bonded rayon varies from little change to high swenlling.

CUPRAMMONIUM SWELLING :


Cameron and morton's test; a few threads of cellulose rayon are shaken in Io
c.c. of (15 gms. copper.200 gms. NH3 per litre) for five
hours at room temperature. untreated viscose is completely soluble.
Highly cross bonded celluloses (e.g. one bond per 40 glucose residues)
are largely unchanged in appearance. intermediate cross bonding
(one bond per IOO glucose residues) gives rise to a highly swollen
condition.

WATER SOULBILLITY:

Soluble cold, insoluble hot; cold water solutions gel on heating :
lower methy celluloses. soluble in hot water and dilute alkalis;
higher methyl cellulose. soluble in cold and hot water : sodium
carbocymethyl cellulose. insoluble in water : ethyl cellulose.

LANTHANUM NITRATE TEST;

To a piece o ffabric in a test tube add a few drops conc. hCI, add I C.C.water, warm ten
minutes, decant off, add a few drops of 5 % lanthanum nitrate, add one drop of
( I gm. iodine, 20 gms. KI, in 500 c.c water), add a few drop of 0.880 ammonia; brown
or blue indicates vinyl acetate or cellulose acetate.



(a)To 0'I gm, resin add 7c.c. chloroform, I C.C. glacial acetic acid, 
I C.C. I O% gromine in chloroform, shake, stand in a closed vessel: 
permanent red indicates coumarone or indene. (b) bromine in carbon 
tetrachloride, below O deg. C. gives the dibromide of indene, m.p.
31.5-32.5 deg. C. which is converted by boiling water into hydroxy-
fromide, m.p. 130'5 deg.C.:



Place a little fabric in I.C.C. of (0'0I% azobenzene phenylhydrazine 
sulphonic acid in IOO c.c. water) add 04 c.c. H2 SO4,heat in a 
steam bath for two to three minutes, cool , add a few drops of pure 
indicates a aldehyde.:



Sunday, January 2, 2011

ANALYTICAL TESTS:

Xanthydrol test 

     The following test is given by the textile Institute ( Tentative Textile specification No.13). Hydrolyse the resin by warming at 50-60deg. C.
a small sample of the fiber in N / IO H2SO4 for a few minutes. Reduce the acidity in the usual way with sodium acetate and ass 1.5 c.c. glacial acetic acid. Add a few drops of IO %solution of xanthyrdol in methyl alcohol to I c.c of the aqueous hydrolysate. which may take some hours to form if only small amounts of urea or thiourea are present.

Vinyl Alcohol Test :
     Reflux the resin or treated cloth with methyl alcoholic KOH (N/2 concentration), filter, concentrate the solution to precipitate polyvinyl alcohol; filter, dissolve the precipitate in water, and acidify, when a blue co lour indicates polyvinyl alcohol.

Reducing Tests :
    (@) Fehilng's Solution: see pp. 42 and 44.
(b) Benedict's qualitative solution : see p.241.
Of these two methods, the Benedict soultion is much to be preferred for qualitative work, because it is stable as a single solution over long periods if kept in a stoppered bottle ,and is always resdy for use; moreover, some indication of the amount of sufar present may be obtained from the colour obtained, which ranges from green to red, with increasing amounts of glucose.

Basic Lead Acetate Test: 
    The reagent is made by pasting 30 gms. lead acetate, IO gms.litharge, with 5 c.c.water; stir stir on water -bath intl white, stir in IOO c.c.water , settle ,and filter. the test consists of adding a few drops of reagnt to a solution of the extract from cloth: a precipitate indicates gum,
moss, or albumen.
  

ANALYTICAL TESTS:

Burning test:

   A small portion of cloth treated with synthetic resin is held to a Bunsen flame, and withdrawn after ignition. This
test is of most value with coated fabrics on which there is a substantial amount of coating. When only small percentages of resin are present, indications are often rather vague. Cellulose nitrate is very inflammable. Rubber has a characteristic odour.  Oxidised oil burns with a fatty smell. The various odours indicated in test 3 may be recognised under favorable circumstances.

Saturday, January 1, 2011

WOOL QUALITY :

WOOL QUALITY:


It is frequently desirable to determine the quality of wool used in the blend from which a yarn or fabric the been made. Results of sufficient accuracy may be obtained by fiber-diameter measurements.
The general division of wool qualities is into merino, crossbred,and cares grades.   Spanish merino is probably the best type of wool: crosses of this with native varieties have given various" crossbreds" and of these the best is botany wool. Of English wool, the coarsest ( longest staple ) are Lincoln,Leicester, Cots wold, Romney Wansley-dale ,and Devon; medium wools are south down, Shropshire, Hampshire, oxford, Suffolk downs, sorts, Rowns, sorest, and Ryland.There are various very coarse wools, used for carpers, on rained mainly from Iran, India, China and Mongolia, these contain unusually large amounts of hair and beard fibers.

infinix hot 6 pro frp bypass without pc in hindi || infinix x608 remove...

subscribe krdo friends 100 subscriber krne hain ples aur ik bar video b dekh lo ap ki aur mari help ho jia ge?